Skip to content
Tactiverge

School/□ Systems Engineer/Elective · MECH-420

Fatigue: failure by a million small pushes

A paperclip survives one bend easily, yet snaps after twenty. Nothing pushed harder the twentieth time. So what broke it?

About 40 min · 3 goals · Checked by automated tests

Review status: Technically checked (automated tests)Content file last checked 2026-11-29.How independent review works

1.Why should I care?

Most mechanical parts that break in service break by fatigue: axles, crankshafts, bike frames, aircraft skins, robot joints that flex millions of times. Each load is safe on its own, but repeated loads grow a tiny crack from a scratch, hole or sharp corner until what is left suddenly fails. Fatigue is why aircraft are inspected on a schedule and why designers fear sharp corners.

  • ◇ Describe fatigue as crack growth under repeated stress well below the static strength.
  • ◇ Read an S–N curve on log axes and explain an endurance limit.
  • ◇ Apply a stress-concentration factor K_t and Miner's rule to a simple load history.

2.Predict

A steel shaft is cycled at a stress amplitude well below its yield stress. Then a small sharp groove is cut into it. What happens to its fatigue life?

Guess first. Being wrong here is how the surprise works.

3.Discover

Set a nominal stress of 150 MPa and K_t = 1: the steel-like part never fails, the aluminium-like part does. Now raise K_t to 2. Use the cycles slider to see how Miner's damage sum grows towards 1.

Loading the interactive…

Can't use the interactive? Read a description instead

The S–N explorer plots stress amplitude (50–600 MPa) against cycles to failure (10³ to 10⁹) on log–log axes. A solid steel-like line falls from 450 MPa at 10³ cycles to 250 MPa at 10⁶ and then stays flat (the endurance limit). A dashed aluminium-like line falls from 280 MPa at 10³ to 120 MPa at 10⁷ and keeps falling. A slider sets the nominal stress amplitude (60–400 MPa) and buttons set the stress-concentration factor (1, 1.5, 2 or 3); a dotted line marks the resulting peak stress. A second slider sets the number of cycles (100,000 to 5,000,000), and the readout gives the predicted life of each part and the Miner's rule damage sum. At 150 MPa with K_t = 2, the steel-like part lasts about 117,000 cycles.

4.Checkpoint: guided practice

Check what you just discovered before going on. Hints appear after a wrong answer.

Practice 1

Can a part fail by fatigue if every load cycle keeps the stress below the yield stress?

Practice 3 · a fresh version every time

A bracket sees three stress levels. At level A it would last 40,000 cycles and sees 6,000; at level B it would last 600,000 and sees 80,000; at level C it would last 6,000,000 and sees 400,000. What is the Miner's rule damage sum D? (3 decimal places)

5.Watch

→ Watch for the three stages: crack initiation at a stress raiser, slow crack growth (beach marks), then sudden final fracture.

Why parts fail after many small loads, and how S–N curves predict fatigue life.

8 min 22 s · captions on YouTube · source

Nothing loads from YouTube until you press play.

The video is optional: everything you need is also in the lesson text and the interactive.

6.Understand

Cracks grow one cycle at a time

Under repeated loading, tiny slips at the most stressed spot start a microscopic crack, usually at the surface, a scratch, a hole or a sharp corner. Each cycle opens and closes it and it grows a little. The part looks fine until the remaining cross-section is too small and it breaks suddenly. Fatigue fractures often show smooth 'beach marks' where the crack grew, and a rough zone where it finally let go.

S–N curves on log axes

Testing many samples at different stress amplitudes S gives the number of cycles to failure N. Plotted on log–log axes, the data scatter around a roughly straight line in the middle region: a small drop in stress buys a big increase in life. Many steels flatten out at an endurance limit (very roughly half the tensile strength for smooth samples): below it, failure is not expected. Aluminium alloys have no true endurance limit and keep weakening.

Stress concentrations

Holes, keyways, threads and sharp internal corners make the local stress higher than the nominal value: σ_peak = K_t × σ_nominal. A round hole in a wide plate in tension has K_t ≈ 3. Because S–N curves are steep, K_t matters far more for fatigue than for a single static load. Generous fillet radii, polished surfaces and moving holes away from high-stress regions are fatigue design.

Miner's rule for mixed loads

Real parts see a mix of stress levels. Miner's rule says each block of nᵢ cycles at a level whose life is Nᵢ uses up a fraction nᵢ/Nᵢ of the part's life, and failure is predicted when D = Σ nᵢ/Nᵢ = 1. It ignores the order of the loads and fatigue scatter is large, so designers aim for D well below 1.

Explain it another way

Fatigue is like a rope fraying one strand at a time. Each pull is fine, but each one breaks a strand, and eventually the last strands go at once.

Worked example 1

A steel-like part (illustrative curve through 10³ cycles at 450 MPa and 10⁶ at 250 MPa, endurance limit 250 MPa) sees 150 MPa nominal. A hole with K_t = 2 is drilled in the most stressed spot. Estimate its life before and after.

Before: 150 MPa < 250 MPa, below the endurance limit, so no fatigue failure is predicted. After: σ_peak = 2 × 150 = 300 MPa. log N = 3 + 3 × log(450/300)/log(450/250) = 3 + 3 × 0.1761/0.2553 ≈ 5.07, so N ≈ 117,000 cycles. One hole turned 'forever' into about a hundred thousand cycles.

Worked example 2

A bracket sees 20,000 cycles at a level where it would last 50,000, and 300,000 cycles at a level where it would last 1,000,000. Use Miner's rule.

D = 20,000/50,000 + 300,000/1,000,000 = 0.4 + 0.3 = 0.7. The rule predicts the bracket survives with 30 % of its life left, but fatigue data scatter by a factor of several in life, so a designer would want D well below 1.

Common mix-ups

  • If a part survives the maximum load once, it will survive it forever.
    ✓ Fatigue depends on the number of cycles. A load that is safe once can grow a crack over thousands or millions of repetitions.
  • Small holes and scratches don't matter because they remove so little material.
    ✓ They are stress raisers. K_t multiplies the local stress, and because S–N curves are steep that can cut fatigue life by orders of magnitude.
  • Miner's rule gives an exact failure point.
    ✓ It is a simplified linear rule that ignores load order and scatter. Real lives can differ by a factor of several, so designers keep D well below 1.

7.Practice on your own

Practice, not a test. Wrong answers get a hint and another try.

Practice 2 · a fresh version every time

A simplified S–N curve for a part is a straight line on log–log axes through (10³ cycles, 350 MPa) and (10⁶ cycles, 160 MPa). At a stress amplitude of 200 MPa, what is log₁₀ of the predicted number of cycles to failure? (2 decimal places)

Practice 4

A plate with a round hole (K_t = 3) carries a nominal stress amplitude of 60 MPa. What is the peak stress amplitude at the edge of the hole, in MPa?

MPa

Practice 5

A robot leg bracket keeps cracking at a sharp inside corner after a few weeks of walking. Which change is most likely to help?

8.Apply it

Pick a part that flexes repeatedly in a machine you know (a door hinge, a bike pedal crank, a robot gripper finger). Estimate how many cycles it sees in a year, sketch where the stress concentrations are, and propose two changes that would extend its fatigue life. Explain each with K_t or the S–N curve.

9.Reflect

Concepts: Stress, strain, materials and safety factors · Reliability, redundancy and failure analysis